SteelHardness (Rc)Toughness (ft-lbs)Austenitize (°F)hold (mins)quenchcryo (hrs)temper (°F)
867059.751.0152510DT-48 oilnone400
867063.96.1152510DT-48 oilnone175
AEB-L59.541.0195015plate0.5350
Z-Finit59.032.3190520plate48895
Z-Finit59.527.8190020plate8325
19C2759.022.8195015plate0.5450
Z-Wear61.922.5195030plate12400
5210061.919.7147510DT-48 oilnone300
CruForgeV61.518.9145010Parks 50 oil0.5400
CruForgeV62.714.4150010Parks 50 oil0.5400
CruForgeV64.013.2150010Parks 50 oil0.5400
CruForgeV66.56.1150010Parks 50 oil0.5300
CPM-15460.518.41950NAplate0.5450
M39061.98.8214010plate12365
CruWear (ingot)60.88.7197530plate12400
40CP60.57.91925NAplate0.5350
Niolox60.57.71975NAplate0.5350
M264.06.2210015plate8400
D261.05.11870NAplate0.5450
N69062.63.7194020plate8175
New Steel59.934.1197515plate0.5350
New Steel61.828.2205015plate0.5350
New Steel63.616.1205015plate0.5300