| Steel | Hardness (Rc) | Toughness (ft-lbs) | Austenitize (°F) | hold (mins) | quench | cryo (hrs) | temper (°F) |
|---|---|---|---|---|---|---|---|
| 8670 | 59.7 | 51.0 | 1525 | 10 | DT-48 oil | none | 400 |
| 8670 | 63.9 | 6.1 | 1525 | 10 | DT-48 oil | none | 175 |
| AEB-L | 59.5 | 41.0 | 1950 | 15 | plate | 0.5 | 350 |
| Z-Finit | 59.0 | 32.3 | 1905 | 20 | plate | 48 | 895 |
| Z-Finit | 59.5 | 27.8 | 1900 | 20 | plate | 8 | 325 |
| 19C27 | 59.0 | 22.8 | 1950 | 15 | plate | 0.5 | 450 |
| Z-Wear | 61.9 | 22.5 | 1950 | 30 | plate | 12 | 400 |
| 52100 | 61.9 | 19.7 | 1475 | 10 | DT-48 oil | none | 300 |
| CruForgeV | 61.5 | 18.9 | 1450 | 10 | Parks 50 oil | 0.5 | 400 |
| CruForgeV | 62.7 | 14.4 | 1500 | 10 | Parks 50 oil | 0.5 | 400 |
| CruForgeV | 64.0 | 13.2 | 1500 | 10 | Parks 50 oil | 0.5 | 400 |
| CruForgeV | 66.5 | 6.1 | 1500 | 10 | Parks 50 oil | 0.5 | 300 |
| CPM-154 | 60.5 | 18.4 | 1950 | NA | plate | 0.5 | 450 |
| M390 | 61.9 | 8.8 | 2140 | 10 | plate | 12 | 365 |
| CruWear (ingot) | 60.8 | 8.7 | 1975 | 30 | plate | 12 | 400 |
| 40CP | 60.5 | 7.9 | 1925 | NA | plate | 0.5 | 350 |
| Niolox | 60.5 | 7.7 | 1975 | NA | plate | 0.5 | 350 |
| M2 | 64.0 | 6.2 | 2100 | 15 | plate | 8 | 400 |
| D2 | 61.0 | 5.1 | 1870 | NA | plate | 0.5 | 450 |
| N690 | 62.6 | 3.7 | 1940 | 20 | plate | 8 | 175 |
| New Steel | 59.9 | 34.1 | 1975 | 15 | plate | 0.5 | 350 |
| New Steel | 61.8 | 28.2 | 2050 | 15 | plate | 0.5 | 350 |
| New Steel | 63.6 | 16.1 | 2050 | 15 | plate | 0.5 | 300 |